Quantified how four heat treatments (normalize, water quench, oil quench, quench + temper) shift the hardness–toughness–strength trade-off in AISI 1045 CD steel
Verified the tensile fixture's bolts were safe at the machine's maximum load
Prepared and stamped dog-bone and Charpy specimens, austenitized at 850 °C, then cooled by the assigned route
Ran Rockwell C hardness (3 indentations per specimen), Charpy impact, and tensile-to-failure testing; pooled results across all lab groups to compare treatments
Calculated bolt shear and bearing safety factors using Von Mises, with Tresca as a conservative check
Mapped the trade-off: water quench 50 HRC / 2.2 ft·lbf / 0.8% elongation; normalizing 16 HRC / 35.6 ft·lbf / 7%
Identified quench + temper as the best operating point, 37 HRC with 18.4 ft·lbf and 175 kpsi UTS
Flagged an anomaly: oil-quenched UTS (180 kpsi) exceeded water-quenched (85 kpsi), likely quench-induced defects causing early brittle fracture
Fixture bolts ran at a shear safety factor of 1.008, effectively at the material's shear limit